What do the numbers in the grade mean?
For QT500-7, the numbers indicate 500 MPa minimum tensile strength and 7% minimum elongation under the specified sample and test conditions. Elongation measures tensile ductility. For an impact requirement, agree the test temperature and required impact energy. Read the table as a guide to grade names, then check the specified edition, sample conditions and applicable wall thickness before setting acceptance values.
| Grade | Comparable EN 1563 grade | Tensile strength (MPa) | Elongation after fracture (%) | Typical matrix and characteristics |
|---|---|---|---|---|
| QT400-15 | EN-GJS-400-15 | 400 | 15 | Usually ferritic, with good ductility. |
| QT450-10 | EN-GJS-450-10 | 450 | 10 | Ferritic or ferritic–pearlitic depending on conditions; a higher nominal strength class than 400-15. |
| QT500-7 | EN-GJS-500-7 | 500 | 7 | Often ferritic–pearlitic, balancing strength and ductility. |
| QT600-3 | EN-GJS-600-3 | 600 | 3 | Often predominantly pearlitic, with higher strength and hardness. |
| QT700-2 | EN-GJS-700-2 | 700 | 2 | Often pearlite-rich, with higher strength and hardness and lower elongation. |
Consider the matrix, hardness and application
Ductile iron properties depend on graphite morphology, the matrix and section conditions. A more ferritic matrix generally offers greater ductility, while pearlite typically increases strength and hardness. The grade designation alone does not specify the matrix proportions or establish properties at a particular point in a casting. Specify hardness, matrix or heat treatment separately when needed.
The table includes comparable EN 1563 designations. Check the sample type, applicable wall thickness and property limits for the specific grade in each standard. Use the same method when comparing with ASTM A536, and specify the governing standard and acceptance criteria in the order.
What to include in a drawing or RFQ
Set the requirements based on the actual loads, section thickness and machining scope.
- Grade and standard · State the complete grade, the standard and its edition. Agree acceptance criteria when comparing grades across standards.
- Test samples and properties · Specify a separately cast coupon, an integrally cast coupon or samples taken from the casting. State the applicable section thickness, sampling location and property requirements.
- Hardness and metallography · When hardness, matrix or nodularity matters, specify the sampling location, assessment method and permitted range.
- Delivery condition · State whether delivery is as cast, annealed, normalized or in another agreed condition.
GB/T 1348 · DIN EN 1563 · ASTM A536
What Wontide can supply
Wontide uses medium-frequency induction melting in Laizhou. Its main business is steel castings and it also reviews ductile iron castings to customer drawings. Its IATF 16949:2016 quality management system certificate covers manufacture of iron and steel castings. In-house tensile, hardness and metallographic testing supports material, mechanical and microstructure reports as agreed.
RFQ checklist · See how to specify nodularity inspection · Cast steel or ductile iron?